“Water repellent” is printed on swing tags, sofa brochures and rug specification sheets everywhere. But when an overseas buyer asks for the spray rating after five washes, or a customer says water still soaks into their cotton cushions, the label alone does not help. You need to know how repellency is actually measured.
This guide explains the three numbers that matter: contact angle, spray rating and wash durability. It is written for makers of furniture, rugs, bedding, curtains and bags, and for applicators checking their work before goods ship.
Key takeaways
- Contact angle shows how strongly a surface sheds a drop, but it is hard to measure reliably on porous, textured fabric.
- The spray test (AATCC 22 or ISO 4920) is the everyday benchmark: a grade from 0 to 100, or 0 to 5.
- Water repellency and oil repellency are separate tests. A fabric can pass one and fail the other.
- A rating means little without the wash count. Always ask for, or quote, results before and after a stated number of washes.
Repellent, resistant or waterproof?
These words are often used as if they mean the same thing. They do not. A water-repellent fabric makes water bead and roll off its surface, while air and vapour still pass through the weave. A water-resistant or waterproof fabric stops water passing through under pressure, which usually needs a membrane or a closed coating.
A repellent finish works at the surface, so the tests below look at how water behaves on the fabric face, not whether rain eventually gets through.
Contact angle: the science behind the bead
Look at a drop of water from the side. The angle between the surface and the edge of the drop is the contact angle. Below 90° the drop spreads and wets the surface. Above 90° it beads. Above about 150° it sits almost as a sphere and rolls away at a slight tilt, which is the “lotus effect”.
On glass or stone, contact angle is a clean, repeatable number. On fabric it is harder. The surface is rough, the yarns are full of gaps, and the drop may slowly sink in while you watch. Instrument makers such as KRÜSS note that fabrics often absorb the test liquid, which is why labs use special set-ups, including the angle at which a drop starts to roll off.
Contact angle suits research and comparing finishes. For quality checks and buyer specifications, the industry relies on the spray test.
The spray test: AATCC 22 and ISO 4920
The spray test is a quick, low-cost way to screen repellency, as AATCC describes it. Under ISO 4920:2012, 250 ml of water is sprayed through a standard 19-hole nozzle onto a taut specimen held at 45°, from 150 mm above its centre. The specimen is tapped to shake off loose drops, then the wetted pattern is compared with written descriptions and reference photos.
| AATCC 22 rating | ISO 4920 grade | What you see on the fabric |
|---|---|---|
| 100 | 5 | No sticking or wetting of the face |
| 90 | 4 | Slight random sticking or wetting |
| 80 | 3 | Wetting at the spray points |
| 70 | 2 | Partial wetting beyond the spray points |
| 50 | 1 | Complete wetting of the face beyond the spray points |
| 0 | 0 | Complete wetting of the entire face |
At least three specimens are tested, so one good swatch is not a result. On dark fabrics, such as navy upholstery or charcoal rugs, the written descriptions carry more weight than the photos.
Oil repellency is a different test
Furniture and rug buyers often ask whether a finish repels oil, not just water. That needs its own method. In AATCC 118, drops of eight test oils, from a heavy mineral oil down to thin n-heptane, are placed on the fabric in turn. The grade, from 0 to 8, is the highest-numbered oil that does not wet the fabric within 30 seconds.
A related method, AATCC 193, uses water and alcohol mixtures to grade resistance to water-based stains such as tea and juice. A PFAS-free finish can score well on the spray test and lower on oil, so check which test a specification means.
Wash durability: the number buyers really want
A fresh finish nearly always looks good. What separates finishes is how much repellency survives washing and use, so a meaningful result pairs a rating with a wash count: for example, as new and after 5, 10 or 20 washes.
Labs use ISO 6330, which sets reference domestic washing and drying procedures. Machine type, detergent and drying all change the outcome, so a report should name the procedure used.
Research on fluorine-free finishes shows why the wash count matters. A 2025 study from the University of Bergamo, published in Polymers, applied a silane and silicone sol-gel finish to cotton and polyester. Both fabrics shed water well, but cotton lost about 15° of contact angle over five washes.
Which test answers which question?
| Test | What it measures | Result | Best used for |
|---|---|---|---|
| Contact angle | How a single drop sits on the surface | Degrees (above 90° = beading) | Research, comparing finishes |
| AATCC 22 / ISO 4920 | Surface wetting under a controlled spray | 0 to 100, or 0 to 5 | Quality control, buyer specs |
| AATCC 118 | Resistance to oily liquids | Grade 0 to 8 | Upholstery, rugs, kitchen textiles |
| AATCC 193 | Resistance to water-based stains | Grade 0 to 8 | Food and drink spills |
| Spray test after ISO 6330 washes | How long repellency lasts | Rating at each wash count | Durability claims, export orders |
Why water still soaks in after treatment
One of the most common questions we hear is some version of “I sprayed my cotton and water still went in”. Check these first:
- Softener or size on the fabric. Silicone softeners, starch and spinning oils sit between the finish and the fibre. Wash or scour first.
- Too little product. The fabric should be evenly damp all over, not misted. Thick rug pile and heavy cotton canvas take more.
- Not enough curing time. Test only after the finish has fully cured, usually 24 hours at room temperature.
- Hard water in the mix. Concentrates should be diluted with deionised water. Much Indian tap and borewell water is hard, which is why deionised water is specified.
A simple in-house check before goods ship
You do not need a laboratory to keep production consistent. Keep a treated and an untreated swatch from each batch and time how long water drops stay round. A basic spray tester built to AATCC 22 dimensions lets you grade swatches yourself, before and after washing.
In the monsoon, let swatches dry and settle indoors before grading. For export orders, agree the target rating, wash count and washing procedure with your buyer in writing.
Where Nanoman Fabric + Textile fits
Nanoman Fabric + Textile is a PFAS-free, water-based finish that uses nanoscale silica to make water bead and roll off without changing how the fabric looks or breathes. It is supplied in 10 litre concentrate cans and diluted 1:19 to 1:39 with deionised water, so you can tune the strength to the fabric and run spray tests on your own swatches at each dilution.
As a guide to how long it lasts in use: clothing 3 to 6 months, shoes and bags about 12 months, carpets and furniture 1 to 2 years, and awnings 2 to 3 years. Our textile protection guide covers application step by step, and our article on PFAS-free water repellents explains how fluorine-free chemistry works.
Frequently asked questions
What is a good spray rating for upholstery fabric?
Higher is better: 100 (ISO 5) means no wetting at all, and 80 (ISO 3) means wetting at the spray points. Buyers set their own targets, usually as a minimum rating after a stated number of washes, so always agree the rating and the wash count together.
Is contact angle or spray rating the better measure?
They answer different questions. Contact angle describes how one drop sits on the surface and suits research. The spray test (AATCC 22 or ISO 4920) reflects real wetting across the fabric face and is the usual basis for specifications.
Why does water soak into my cotton after I sprayed it?
The usual causes are softener or starch left on the fabric, too little product, testing before the finish has cured for 24 hours, or diluting with hard water instead of deionised water. Clean the fabric, reapply evenly and test again after curing.
How long does a water-repellent finish last?
It depends on wear and washing. As a guide, expect 3 to 6 months on regularly washed clothing, about 12 months on shoes and bags, 1 to 2 years on carpets and furniture, and 2 to 3 years on awnings. Reapply when water stops beading.
Need repellency you can measure? Tell us the fabric, the end use and the rating your buyer asks for, and we will suggest a starting dilution to test. We reply within one business day.